化工学报 ›› 2017, Vol. 68 ›› Issue (5): 2148-2154.DOI: 10.11949/j.issn.0438-1157.20161657

• 能源和环境工程 • 上一篇    下一篇

Shell炉合成气冷却器分层积灰特性

韩瑞午, 谭厚章, 魏博, 王毅斌, 张朋   

  1. 西安交通大学热流科学与工程教育部重点实验室, 陕西 西安 710049
  • 收稿日期:2016-11-23 修回日期:2017-01-17 出版日期:2017-05-05 发布日期:2017-05-05
  • 通讯作者: 谭厚章
  • 基金资助:

    国家自然科学基金项目(51376147)。

Characteristics of layered ash deposition in Shell coal gasification syngas cooler

HAN Ruiwu, TAN Houzhang, WEI Bo, WANG Yibin, ZHANG Peng   

  1. MOE Key Laboratory of Thermo-Fluid Science and Engineering, Xi'an Jiaotong University, Xi'an 710049, Shaanxi, China
  • Received:2016-11-23 Revised:2017-01-17 Online:2017-05-05 Published:2017-05-05
  • Supported by:

    supported by the National Natural Science Foundation of China (51376147).

摘要:

以某Shell气化炉合成气冷却器严重积灰结垢区域的灰样为研究对象,通过X射线荧光光谱仪、X射线衍射仪、扫描电子显微镜等对其物化特性进行表征,并分析积灰的形成机制。结果表明,灰样内部存在明显的分层结构:最底层呈红色,结晶程度最高且质地坚硬,主要矿物组成有CaSO4、Fe2O3、FeS等;中间层呈黄色,Fe、S含量降低,结晶程度和硬度下降;最外层呈灰色,Fe、S含量最低,为非晶体结构且松软多孔。各灰层间颜色、硬度和内在矿物组分的较大差异,主要是由于在积灰发展过程中,沉积表面温度升高导致沉积层的黏附作用和烧结作用不同。而低熔点含铁矿物的选择性沉积和富集,是初始灰层形成的主要原因。

关键词: 气化, 合成气冷却器, 结垢, 分层结构, 烧结, 初始灰层

Abstract:

Serious ash deposition and fouling from the synthetic gas cooler in Shell gasifier was studied. The physicochemical characteristics of samples were investigated by X-Ray Fluorescence Spectrometer (XRF), X-Ray Diffraction (XRD), Scanning Electron Microscopy and Energy Dispersive Spectrometer (SEM-EDS) respectively to explore the mechanisms of ash accumulation problem. The results showed that the deposition had an obvious layered structure. The inner layer, which presented red color, had the highest degree of crystallization and stiff structure. Its dominant mineral components were calcium sulfate, iron oxide and ferrous sulfide. The middle layer presented yellow color. The amount of Fe and S, the crystallinity and hardness all decreased. The outer layer, which presented grey color and had the lowest amount of Fe and S, was amorphous, soft and porous. The differences of color, hardness and mineral components among three ash layers are due to different interaction of adhesion and sintering as the deposition surface temperature increases with the growth of ash thickness. Ash composition, temperature, reaction atmosphere and pressure are all important factors. And the selective deposition and accumulation of iron-bearing minerals with low melting point in heat transfer surfaces are important sources of initial layer.

Key words: gasification, syngas cooler, fouling, layered structure, sintering, initial layer